45KH14N14V2M (45Х14Н14В2М)
UNS S66009
SUH31
45KH14N14V2M ( 45Х14Н14В2М ) is high alloy high-temperature steel
Equivalent grade
USA | Japan | France | England | Hungary | Poland | Czechia | |||||||
- | JIS | AFNOR | BS | MSZ | PN | CSN | |||||||
|
|
|
|
|
|
|
Chemical composition
C | Si | Mn | Ni | S | P | Cr | Mo | W |
0.4 - 0.5 | max 0.8 | max 0.7 | 13 - 15 | max 0.02 | max 0.035 | 13 - 15 | 0.25 - 0.4 |
2 - 2.8 |
Mechanical properties under Т=20oС for grade
Assortment | Dimension | Direct. | sв | sT | d5 | y | KCU | Heat treatment |
- | mm | - | MPa | MPa | % | % | kJ / m2 | - |
Bar, GOST 5949-75 | 710 | 315 | 20 | 35 | Drawing 810 - 830oC, air, |
Brinell hardness for 45KH14N14V2M ( 45Х14Н14В2М ) (annealing) , Bar GOST 5949-75 | HB 10 -1 = 197 - 285 MPa |
Weldability :
without limitations- welding is done without heating and subsequent heat treeting
limited weldability- welding is possible under heating up to 100-120 grade and subsequent heat treeting
hard weldability- obtaining the quality welding needs the additional operations:heating up to 200-300 grade; the heat treeting ia annealing
Physical properties
T | E 10- 5 | a 10 6 | l | r | C | R 10 9 |
Grade | MPa | 1/Grade | Watt/(m·Grade) | kg/m3 | J/(kg·Grade) | Ohm·m |
20 | 2.08 | 14 | 8000 | 815 | ||
100 | 1.96 | 16 | 875 | |||
200 | 1.9 | 17 | 17 | 7930 | 945 | |
300 | 1.81 | 19 | 507 | 1000 | ||
400 | 1.73 | 18 | 20 | 7840 | 511 | 1055 |
500 | 1.66 | 21 | 523 | 1098 | ||
600 | 1.57 | 18 | 22 | 7760 | 528 | 1142 |
700 | 1.49 | 24 | 1172 | |||
800 | 1.41 | 19 | 7660 | |||
T | E 10- 5 | a 10 6 | l | r | C | R 10 9 |